A buyer approves your 15% post-consumer recycled (PCR) HDPE bottle, then asks for 30% because a retail customer wants a higher recycled claim. The mold, machine and often the resin grade name stay the same, so the tempting answer is to change the ratio and ship. The question is whether the higher share still holds its drop, stack and stress-crack performance. A ratio change is a material change that reopens qualification.
The short answer: requalify at every ratio
Treat each ratio as a new material and requalify it. Melt index, contamination and moisture shift as PCR content rises, so parison sag, wall distribution and ESCR move with them. Rerun drop, stack, ESCR, odour and colour at 0, 15, 30 and 50 percent before releasing a higher ratio.
Why a higher PCR share moves the process window
PCR is a blend of bottle streams, and its history does not stop at the hopper. Four mechanisms matter most.
- Melt index spread. A higher share widens the molecular weight distribution, so the parison sags more. A die gap set on virgin resin may run thin at the neck and heavy at the base.
- Contamination. Gels, specks, adhesive and label residue, and other polymer fragments create weak points in the wall and at pinch-off.
- Moisture. Washed flakes carry surface water; without drying and devolatilization, the result is bubbles, holes and lower melt strength.
- Colour and odour. Ink, adhesive and previous contents vary by bale, so colour drifts between lots and odour can survive the melt.
The container itself is covered inHDPE bottle blow molding, the 25 L case in25 L lubricant oil bottle production, and stack performance inblow molded container stacking.
The 0/15/30/50% trial matrix
Run the ladder on the machine and mold that will make the production part. On a 10 L single-station platform such as the ES-10LS, the 70-75 mm screw and 80-100 kg/h output band set the pace; the double-station ES-10LD runs an 80-90 mm screw at 130-160 kg/h. Those figures describe the extruder, not your PCR. The trial shows how much capacity you can use at each ratio.
Keep everything except the ratio fixed in the first pass: same mold, colour, blow pressure and cooling time. A matrix is only a comparison if one variable moves.
| PCR share | Main risk | What to measure | Release rule |
|---|---|---|---|
| 0% | Virgin reference for every later ratio. | Wall weight, cycle time, drop, stack, ESCR, colour, odour. | Keep a sample and a full record. |
| 15% | Small melt-index shift; occasional gels and specks. | Parison sag, neck and body wall, drop, ESCR, colour. | All five tests pass before a customer trial. |
| 30% | Wider viscosity spread, moisture pick-up, colour drift. | Melt pressure, sag, pinch-off, drop, stack, ESCR, odour, colour. | Full requalification on production-cavity containers. |
| 50% | Highest contamination and sag risk; cycle time may rise. | Screw speed, melt temperature, cycle time, wall, all five tests. | Release on this ratio's measured data only. |
Swipe the table to see all columns →
The five-item requalification checklist
Take containers from the same cavity and shift for every test, and record results per cavity rather than one lot average. For a filled, stacked and shipped HDPE container, these five items are the minimum.
- Drop. Use the customer's protocol: same fill weight, orientation, drop height and surface. Record pass or fail per cavity.
- Stack. Load the customer's pallet pattern and duration. PCR containers creep more, so measure deformation under load.
- ESCR. Fill with the actual product or the specified wetting agent, hold under load and check the pinch-off and neck. Confirm the protocol with your customer or test house.
- Odour. Seal samples, condition them at the filling or storage temperature, and compare with a retained sample from the previous ratio.
- Colour. Measure a fixed point with a colorimeter and keep a physical sample per ratio. Factory light hides drift that a shelf exposes.
Tests only count if each container traces to its material. Keep one batch record per trial: date, machine, mold and cavity, resin lot, PCR supplier and source, ratio, MFI, moisture, colour, settings, measured cycle time, wall weight and test results. That sheet answers a customer question months later.
A worked example: from 15% to 30% on a 10 L container
Take a two-cavity mold and a measured cycle time of 20 seconds at the released 15% ratio. That is 180 cycles per hour, or 360 containers per hour at two good parts. If 30% PCR needs 22 seconds to hold wall thickness, output falls to about 327 per hour, roughly 9% less. The number is an example: measure the cycle at each ratio and recalculate.
The extruder sets the second limit. The ES-10LS is rated 80-100 kg/h and the ES-10LD 130-160 kg/h. A heavier wall at a higher PCR share raises kilograms per hour even as output falls, so watch melt pressure and screw recovery.
What to send for a quotation
A machine quotation cannot certify a PCR ratio, but it can be specified for the trial that will qualify it. Send these with the inquiry:
- Container drawing in 2D and 3D, with neck finish, wall map and target weight.
- Resin grade and PCR source: supplier, bottle stream, collection country and MFI certificate.
- The ratio ladder you plan to qualify, such as 0/15/30/50 percent, and which levels are customer requirements.
- The five test protocols: drop height and fill, stack load and duration, ESCR medium, odour reference and colour tolerance.
- Output target, shift pattern, and available power, compressed air and cooling water.
- Mold status, cavity count, the machine running the virgin version, and the destination market.
Send the drawing and trial plan through thecontact page, and compare the0.1-16 L single-station rangewith thedouble-station platformbefore fixing a model.
Source: E-SHION product data. Specifications are subject to change without notice; customization is available.
This guide is written for production and procurement decisions. It uses published figures where available and avoids unverified performance claims.