A colour that passes on a chip and fails on the bottle is one of the quietest ways to lose money in blow molding. The pigment has not changed. The resin, the wall thickness, the surface and the light it is judged under have. Approve colour the wrong way and every shipment reopens the same argument about which bottle is the reference.

Approve the bottle, not the chip

Colour is approved on a container blown from the final resin, at the final wall thickness and surface finish. A chip, a plaque or a bottle from another machine only tells you what the pigment looks like. The approval itself is a written rule: light source, Delta E, gloss, opacity, limit samples, resin and regrind.

Three variables move the colour before the pigment reaches the mold. Resin: the same masterbatch dosed into two HDPE grades with different base colour and haze gives two different bottles. Wall thickness: a translucent container reads darker where the parison is thick and lighter where it is stretched, so a colour matched on a thin test bottle will not hold on a heavy handle bottle. Surface: gloss, texture and mold finish change how light leaves the wall.

  • The base resin and its own colour and haze
  • Wall thickness on the neck, body and base
  • Gloss, texture and mold finish
  • Pigment dispersion, which shows on a stretched wall
  • The light source, which can hide a metameric match

The colour approval sheet: six items to agree in writing

A signed bottle is not a specification. Put the colour rule on one page that both sides sign, so a new shift, a new resin lot or a new mold can be checked against it without a phone call. These are the six items that decide whether a colour complaint is a real defect or a matter of opinion.

Colour approval sheet: what both sides sign before the first production run
Item What to record Why it matters
Light sourceD65 as the standard viewing condition, plus any second source used for a checkA match under one light can shift under shop or warehouse lighting
Delta E limitOne agreed figure for the container, with a tighter figure if the brand asks for itA tolerance is a decision, not a default, and must be written before the first run
Gloss and opacityMeasured gloss level, and whether the wall is opaque, translucent or clearGloss and opacity move perceived colour more than a small pigment change
Limit samplesTwo signed containers: the lower and upper edge of acceptable colourOne sample cannot show a range, so every batch becomes an argument
Resin and regrindResin grade, masterbatch code, let-down ratio and regrind percentageColour is only repeatable if the formula behind it is fixed
Reading pointsNeck, body and base read separately, not as one averageWall thickness varies by position, and one reading hides a two-tone bottle

Swipe the table to see all columns →

5L Jerrycan Blow Molding Machine | Mold and Container Take-Off A representative 5l jerrycan blow molding machine | mold and container take-off clip. The machine, mold and configuration in your project may differ.

Masterbatch ratio, screw mixing and regrind

The trial that settles most colour arguments is small. Run the same mold at 2% and 4% masterbatch let-down, each with 0% and 20% regrind, and read the neck, body and base of every container against the signed limit samples. Four combinations and three reading points per bottle show whether the colour survives the regrind loop and whether the screw disperses the masterbatch evenly. If the colour drifts at 20% regrind, the problem is the ratio in the spec, not the pigment.

Dispersion is a machine setting as much as a pigment property. Screw geometry, back pressure, melt temperature and residence time decide how evenly the colour is distributed. Streaks and swirls on the body usually point to dispersion or dose rate; a colour that is uniformly wrong points to pigment choice or let-down ratio.

Regrind is the usual reason a colour approved in January fails in June. Write a maximum regrind percentage into the production spec, keep regrind from other colours out of the loop, and expect a dark run to carry pigment into the next light one. The 0% and 20% trial above is how you find the ceiling for your own bottle.

Pigment, UV package and food contact

Colour and UV protection are not separate purchases. A UV absorber or HALS package added to protect the container outdoors can interact with the pigment, and a pigment that is fine in an opaque wall may behave differently in a thin translucent one. Migration and food-contact status belong in the approval, not in a supplier email after the first shipment.

  • Ask for the pigment's migration and food-contact status in writing, for the resin and the intended filling, not for a generic grade
  • Confirm the UV package is compatible with the pigment before the trial, not after the first outdoor batch
  • State whether the colour is through-colour or a surface effect, because the two fail in different ways
  • Check food-contact status against the actual product, not against water

Colour sits inside a wider resin decision. If recycled content is part of the project, therecycled content packaging rulesexplain what has to be declared, and for clear containers thePETG bottle temperature rangecovers the processing window that affects clarity.

What to send for a quotation

A colour quotation is only as good as the information behind it. Send these six items and the machine, mold and trial plan can be quoted in one pass.

  • Container drawing: volume, neck finish, target wall thickness, handle and base detail
  • Resin grade and base colour, plus the regrind percentage you intend to run
  • Masterbatch code, let-down ratio, and the colour target with its Delta E limit and light source
  • Surface requirement: gloss level, texture, opaque, translucent or clear, and any decoration
  • UV or food-contact requirement, with the standard the container must meet
  • Destination, drive and control preference, and expected output per hour

The trial runs on the machine that will make the bottle, so station count matters: compare thesingle-station 0-16 L serieswith thedouble-station 0-16 L series, or send the drawing throughcontact.

Source: E-SHION product data. Specifications are subject to change without notice; customization is available.

This guide is written for production and procurement decisions. It uses published figures where available and avoids unverified performance claims.